Peopoly Phenom XXL Resin Settings for 3DRS Resins

On the Peopoly Phenom XXL, start 3DRS HERO HD Medium Grey at 10.6 s per layer at 50 microns, RPG at 13.9 s and Standard HD Dark Cool Grey at 20.0 s. Use 6 burn in layers at 62.3 s. Every resin colour has its own card below with 30, 50 and 100 micron values.

Last updated November 2, 2026. Starting values; adjust 0.1 to 0.2 s for your printer and conditions. Values come from the 3DRS settings sheet, testing by The 3DRS Team and our research on each printer. Questions? Contact us.

  • Release: Single stage lift
  • Screen: 3840 x 2160
  • XY pixel: 137.2 µm
  • Build volume: 527 x 296.5 x 550 mm
  • File format: ctb, cbddlp

HERO HD RPG Standard HD Platinum Cure Cast Lift and retract FAQ All printers

HERO HD settings on the Peopoly Phenom XXL

HERO HD Medium Grey

HERO HD Medium Grey exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer10.4 sRange 10.3 to 10.5 s
  • 50 µm layer10.6 sRange 10.5 to 10.7 s
  • 100 µm layer11.6 sRange 11.5 to 11.7 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 62.3 s, 4 transition layers

Shop HERO HD Medium Grey

HERO HD Light Grey

HERO HD Light Grey exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer11.1 sRange 11.0 to 11.2 s
  • 50 µm layer11.3 sRange 11.2 to 11.4 s
  • 100 µm layer12.3 sRange 12.2 to 12.4 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 62.3 s, 4 transition layers

Shop HERO HD Light Grey

HERO HD Pearl White

HERO HD Pearl White exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer12.7 sRange 12.6 to 12.8 s
  • 50 µm layer12.9 sRange 12.8 to 13.0 s
  • 100 µm layer13.9 sRange 13.8 to 14.0 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 62.3 s, 4 transition layers

Shop HERO HD Pearl White

HERO HD Sienna

HERO HD Sienna exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer12.1 sRange 12.0 to 12.2 s
  • 50 µm layer12.3 sRange 12.2 to 12.4 s
  • 100 µm layer13.3 sRange 13.2 to 13.4 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 62.3 s, 4 transition layers

Shop HERO HD Sienna

HERO HD Merchant Grey

HERO HD Merchant Grey exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer12.1 sRange 12.0 to 12.2 s
  • 50 µm layer12.3 sRange 12.2 to 12.4 s
  • 100 µm layer13.3 sRange 13.2 to 13.4 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 62.3 s, 4 transition layers

Shop HERO HD Merchant Grey

HERO HD Flesh

HERO HD Flesh exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer12.1 sRange 12.0 to 12.2 s
  • 50 µm layer12.3 sRange 12.2 to 12.4 s
  • 100 µm layer13.3 sRange 13.2 to 13.4 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 62.3 s, 4 transition layers

Shop HERO HD Flesh

RPG settings on the Peopoly Phenom XXL

RPG Medium Grey

RPG Medium Grey exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer13.7 sRange 13.6 to 13.8 s
  • 50 µm layer13.9 sRange 13.8 to 14.0 s
  • 100 µm layer14.9 sRange 14.8 to 15.0 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 71.2 s, 4 transition layers

Shop RPG Medium Grey

Standard HD settings on the Peopoly Phenom XXL

Standard HD Dark Cool Grey

Standard HD Dark Cool Grey exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer19.8 s
  • 50 µm layer20.0 s
  • 100 µm layer21.0 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 80 s, 4 transition layers

Shop Standard HD Dark Cool Grey

Standard HD Flat Grey

Standard HD Flat Grey exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer15.1 sRange 15.0 to 15.2 s
  • 50 µm layer15.3 sRange 15.2 to 15.4 s
  • 100 µm layer16.3 sRange 16.2 to 16.4 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 6 layers at 80 s, 4 transition layers

Shop Standard HD Flat Grey

Platinum Cure Cast settings on the Peopoly Phenom XXL

These are starting values based on customer reports and similar clear resin data. Run a test print or exposure test first.

Platinum Cure Cast Clear

Platinum Cure Cast Clear exposure and burn in settings on the Peopoly Phenom XXL, by layer height

Normal layer exposure, starting value

  • 30 µm layer16.7 sRange 16.6 to 16.8 s
  • 50 µm layer16.9 sRange 16.8 to 17.0 s
  • 100 µm layer17.9 sRange 17.8 to 18.0 s

Adjust 0.1 to 0.2 s as needed.

Burn in: 5 layers at 20 s, 5 transition layers

Printing directly on the build plate with no supports? Use about 3 s for 5 burn in layers, with 5 transition layers.

Shop Platinum Cure Cast Clear

Platinum Cure Cast Clear lift, retract and wait settings on the Peopoly Phenom XXL

Burn in layers

Lift distance, stage 1 (mm)
15
Retract distance, stage 1 (mm)
15
Lift speed, stage 1 (mm/min)
32
Retract speed, stage 1 (mm/min)
100
Wait before print (s)
0
Wait after print (s)
0
Wait after lift (s)
0
Light intensity (%)
100

Normal layers

Lift distance, stage 1 (mm)
14
Retract distance, stage 1 (mm)
14
Lift speed, stage 1 (mm/min)
35
Retract speed, stage 1 (mm/min)
100
Wait before print (s)
1
Wait after print (s)
0
Wait after lift (s)
0
Light intensity (%)
100

Platinum Cure Cast print and bake tips

Before you print

  • Settings assume supported prints. With supports, keep the burn in exposure at or under 15 to 20 s.
  • If you print directly on the build plate, use a short burn in of about 3 s for 5 layers with 5 transition layers.

Orientation

  • Print parts at an angle. Large flat areas facing the plate can cup and leave defects.
  • Clear resin can close small holes, most of all holes that run along the Z axis. Orient parts so critical holes do not run straight up.
  • Very small columns are hard to hold. If they fail, slow the lift speed, add a short rest and raise the exposure a little.
  • Take care with thin walls, which can distort.

Post processing (required)

  1. Wash thoroughly in IPA.
  2. Let the part dry completely, overnight or with compressed air and about 3 hours of drying. Parts that are still wet can show surface problems.
  3. UV cure for 10 to 20 minutes.
  4. Bake at 275°F (135°C) for 60 to 80 minutes in a dedicated oven or air fryer, never a kitchen oven used for food.

The bake is what lets platinum silicone cure against the printed part. Without it the silicone will stay uncured where it touches the print.

Limits

  • Made for open molds used with platinum cure silicone.
  • Not recommended for closed or injected molds. In testing, injected silicone stayed uncured even after repeated cure cycles.

Lift, retract and wait settings for the Peopoly Phenom XXL

The maker profile uses a single stage lift, so only stage 1 values are listed. Field names follow Lychee Slicer. Use the same values in the matching fields of your slicer.

Lift, retract and wait settings on the Peopoly Phenom XXL for HERO HD, RPG and Standard HD (Lychee field names)

Burn in layers

Lift distance, stage 1 (mm)
15
Retract distance, stage 1 (mm)
15
Lift speed, stage 1 (mm/min)
32
Retract speed, stage 1 (mm/min)
100
Wait before print (s)
0
Wait after print (s)
0
Wait after lift (s)
0
Light intensity (%)
100

Normal layers

Lift distance, stage 1 (mm)
14
Retract distance, stage 1 (mm)
14
Lift speed, stage 1 (mm/min)
35
Retract speed, stage 1 (mm/min)
100
Wait before print (s)
1
Wait after print (s)
0
Wait after lift (s)
0
Light intensity (%)
100

Peopoly Phenom XXL resin settings FAQ

What exposure should I use for 3DRS HERO HD on the Peopoly Phenom XXL?

At 50 microns, start HERO HD Medium Grey at 10.6 s, Light Grey at 11.3 s and Pearl White at 12.9 s. Adjust 0.1 to 0.2 s as needed after a calibration print.

How many burn in layers should I use on the Peopoly Phenom XXL?

For HERO HD Medium Grey at 50 microns, use 6 burn in layers at 62.3 s, followed by 4 transition layers.

What lift and retract settings work on the Peopoly Phenom XXL?

For normal layers, lift 14 mm at 35 mm/min and retract at 100 mm/min. The lift and retract settings above list burn in values too.

What about RPG and Standard HD on the Peopoly Phenom XXL?

At 50 microns, start RPG Medium Grey at 13.9 s, Standard HD Dark Cool Grey at 20.0 s and Standard HD Flat Grey at 15.3 s.

What settings should I use for Platinum Cure Cast on the Peopoly Phenom XXL?

At 50 microns, start Platinum Cure Cast Clear at 16.9 s with 5 burn in layers at 20 s. These are starting values based on customer reports and similar clear resin data, so run an exposure test first. After printing, wash in IPA, dry fully, UV cure for 10 to 20 minutes and bake at 275°F (135°C) for 60 to 80 minutes before casting platinum silicone.

Need help dialing in your Peopoly Phenom XXL?

Email info@3dresinsolutions.com with your printer, resin and layer height. See settings for other printers.